Specifications
Surface Treatments
Certifications
- ISO 9001 - 2015 Certified
- PED 2014/68/EC
- NACE MR0175/ISO 15156-2
- NORSOK M-650
- DFAR
- MERKBLATT AD 2000 W2/W7/W10
Standard Austenitic Stainless Steel Bolts, Stud Bolts, Screws, Nuts & Washers in EN 10269 Grade X5CrNi18-10 (1.4301)
EN 10269 Grade X5CrNi18-10 (1.4301) Fasteners are standard austenitic stainless steel fasteners equivalent to AISI 304, offering good general corrosion resistance, formability, and performance in a wide range of corrosive environments, used in pressure vessels, chemical equipment, food processing, and marine applications.
| Material designation | Chemical composition, % by mass | ||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Name | Number | C | Si | Mn | P max. | S max. | Al tot | B | Cr | Mo | Ni | V | Others |
| Steels for quenching and tempering | |||||||||||||
| X5CrNi18-10 | 1.4301 | ≤ 0,07 | ≤ 1,00 | ≤ 2,00 | 0.045 | 0,015 b | - | - | 17,0 to 19,5 | - | 8,0 to 10,5 | - | N ≤ 0,10 |
|
|||||||||||||
| Material designation | Heat treatment conditiona | Diameter c | Proof strength | Tensile strength | Elongation after fracture | Reduction in area | Impact energy (ISO-V) at 20°C | |
|---|---|---|---|---|---|---|---|---|
| Name | Number | |||||||
| d mm | Rp0,2 MPa min. | Rm MPa | A % min. | Z % min. | KV2 J min. | |||
| X5CrNi18-10 | 1.4301 | +AT | d< 160 | 190 | 500 to 700 | 45 | - | 100 |
| +C700 | d ≤ 35 | 350 | 700 to 850 | 20 | - | 80 | ||
|
||||||||
| Material designation | Heat treatment conditiona | Diameter e d mm | Minimum 0,2 %-proof strength Rp0, 2 in MPa at a temperature (in °C) of: |
|||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Name | Number | 50 | 100 | 150 | 200 | 250 | 300 | 350 | 400 | 450 | 500 | 550 | 600 | 650 | ||
| X5CrNi18-10 | 1.4301 | +AT | d ≤ 160 | 177*) | 155 | 140 | 127 | 118 | 110 | 104 | 98 | 95 | 92 | 90 | - | - |
|
||||||||||||||||
| Material designation | Heat treatment conditiona | Diameter c d mm | Minimum tensile strength Rm in MPa at a temperature (in °C) of: |
|||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Name | Number | 50 | 100 | 150 | 200 | 250 | 300 | 350 | 400 | 450 | 500 | 550 | 600 | 650 | ||
| X5CrNi18-10 | 1.4301 | +AT | d ≤ 160 | 480 | 450 | 420 | 400 | 390 | 380 | 380 | 380 | 375 | 360 | 335 | 300 | - |
|
||||||||||||||||
| Material designation | Heat treatment conditiona | Diameter e d mm | Minimum impact energy KV2 in J c (ISO-V test piece) at a test temperature in °C of: |
||||||||||||||||
|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|---|
| Name | Number | -270 | -196 | -160 | -140 | -120 | -110 | -100 | -90 | -80 | -70 | -60 | -50 | -40 | -20 | 0 | +20 | ||
| X5CrNi18-10 | 1.4301 | +AT | d ≤ 160 | - | 60 | - | - | - | - | - | - | - | - | - | - | - | - | - | 100 |
| +C700 | d ≤ 35 | - | 50 | - | - | - | - | - | - | - | - | - | - | - | - | - | 80 | ||
|
|||||||||||||||||||